牌號 | X3CrTi17 |
1.4510 | |
對應標準 | NF EN 10028-7-2008
壓力容器用不銹鋼扁平產(chǎn)品 Flat products made of steels for pressure purposes - Part 7 : stainless steels |
歸類 | 鐵素體不銹鋼 |
Material designation | Heat treatment condition | Minimum 0.2% proof strength Rp0.2,MPa at a temperature (in°C) of: | ||||||||
Name | Number | 50① | 100 | 150 | 200 | 250 | 300 | 350 | 400 | |
X3CrTi17 | 1.4510 | +A | 223 | 195 | 190 | 185 | 175 | 165 | 155 | - |
① Determined by linear interpolation. |
Material designation | Hot forming | Heat treatment symbol | Anneailing | |||
Name | Number | Temperature ℃ | Type of cooling | Temperature① ℃ | Type of cooling | |
X3CrTi17 | 1.4510 | 1100 to 800 | air | +A | 770 to 830 | air,water |
◎ a=air; o=oil; w=water. ◎ The temperatures of annealing should be agreed for simulated heat treated test pieces. ① If heat treatment is carried out in a continuous furnace, the upper part of the range specified is usually preferred, or even exceeded. |