牌號(hào) | X2CrNiMoN22-5-3 |
1.4462 | |
對(duì)應(yīng)標(biāo)準(zhǔn) | NF EN 10028-7-2000
壓力容器用不銹鋼扁平產(chǎn)品 Flat products made of steels for pressure purposes Part 7: Stainless steels |
歸類(lèi) | 雙相不銹鋼 |
Material designation | Heat treatment condition | Minimum 0.2% proof strength Rp0.2,MPa at a temperature (in°C) of: | |||||
Name | Number | 100 | 150 | 200 | 250 | ||
X2CrNiMoN22-5-3 | 1.4462 | +AT | 360 | 335 | 315 | 300 |
Material designation | Heat treatment condition | Minimum tensile strength,MPa at a temperature (in°C) of: | |||||
Name | Number | 100 | 150 | 200 | 250 | ||
X2CrNiMoN22-5-3 | 1.4462 | +AT | 590 | 570 | 550 | 540 |
Material designation | Hot forming | Heat treatment symbol | Solution anneailing ① | |||
Name | Number | Temperature ℃ | Type of cooling | Temperature ℃ ② | Type of cooling | |
X2CrNiMoN22-5-3 | 1.4462 | 1150 to 950 | air | +AT | 1060 ± 40 | water,air |
◎ a=air; o=oil; w=water. ◎ The temperatures of annealing should be agreed for simulated heat treated test pieces. ① Solution annealing in the range specified followed by sufficiently rapid cooling to avoid precipitation of deleterious phases is essential after hot forming these steets. ② If heat treatment is carried out in a continuous furnace, the upper part of the range specified is usually preferred, or even exceeded. |