牌號(hào) | GX40NiCrSi35-25 |
德國(guó)W-Nr. | 1.4857 |
對(duì)應(yīng)標(biāo)準(zhǔn) | DIN 17465-1993
耐熱鑄鋼 Heat resisting steel castings - Technical delivery conditions |
歸類 | 鑄鋼 |
標(biāo)簽 | 奧氏體型耐熱鑄鋼 最高工作溫度1100°C |
Material | 1% creep limit after 10000 h, in N/mm2, at a temperature, in °C, of | Maximum service temperature, in °C | ||||||
designation | number | 600 | 700 | 800 | 900 | 1000 | 1100 | |
GX40NiCrSi35-25 | 1.4857 | - | 70 | 40 | 20 | 8 | 2 | 1100 |
Material | Den- sity, in g/cm3 | Thermal con- ductivity, in W/K.m | Specific heat capacity at 20 °C, in J/g.K | Coefficient of linear thermal expansion, in 10-6 /K, at a temperature between 20 °C and | |||
designation | number | 400 °C | 800°C | 1000°c | |||
GX40NiCrSi35-25 | 1.4857 | 8 | 14.6 | 0.50 | 15.5 | 17.0 | 18.0 |
Material | suitable fillet metal | Heat treatment | ||||
designation | number | Covered electrode (symbol) | Wire or rod (symbol) | Material number | prior to welding | after welding |
GX40NiCrSi35-25 | 1.4857 | 25 35Nb | X40NiCrNb35-25 | 1.4853 | - | - |